In this work, the activated carbon was prepared from biowaste of Eichhornia crassipes by chemical activation method using KOH as the activating agent at various carbonization temperatures (600 °C, 700 °C and 800 °C). The disordered nature, morphology and surface functional groups of ACs were examined by XRD, SEM and FT-IR. The electrochemical properties of AC electrodes were studied in 1M H2SO4 in the potential range of -0.2 to 0.8 V using cyclic voltammetry (CV), galvanostatic charge-discharge and electrochemical impedance spectroscopy (EIS) techniques in a three electrode system. Subsequently, the fabricated supercapacitor using AC electrode delivered the higher specific capacitance and energy density of 509 F/g at current density of 1 mA/cm2 and 17 Wh/kg at power density of 0.416 W/g.